Materialvergleich des ASTM A 199-Wärmetauscherrohrs
|
ASTM-Standard |
japanisch |
Deutsch |
britisch |
||
|
JIS-Nr |
DIN-Typ |
DIN-Nr |
BS-Nr |
BS-Note |
|
|
A199 T5 |
STBA25 |
12crmo19 5 |
3606 |
CFS625 |
|
|
A199 T11 |
STBA23 |
DIN17175 |
13crmo44 |
3606 |
CFS621 |
|
A199 T22 |
STBA24 |
SEW610 |
10crmo9 10 |
3606 |
CFS622 |
|
A199 t9 |
STBA26 |
DIN17175 |
12CrMo195 |
3606 |
|
Chemische Analyse von ASTM A199 (%):
|
Stahlsorte |
C |
Mn |
P (maximal) |
S (maximal) |
Si |
Cr |
Mo |
|
ASTM A199 T4 |
0,15MAX |
0.30-0.60 |
0.03 |
0.03 |
0.50-1.0 |
2.15-2.85 |
0.44-0.65 |
|
ASTM A199 T5 |
0.50-0.15 |
0.30-0.60 |
0.03 |
0.03 |
0,50MAX |
4.00-6.00 |
0.45-0.65 |
|
ASTM A199 T9 |
0,15MAX |
0.30-0.60 |
0.03 |
0.03 |
0.25-1.0 |
8.00-10.0 |
0.90-1.10 |
|
ASTM A199 T11 |
0.50-0.15 |
0.30-0.60 |
0.03 |
0.03 |
0.50-1.0 |
1.00-1.50 |
0.44-0.65 |
|
ASTM A199T22 |
0.50-0.15 |
0.30-0.60 |
0.03 |
0.03 |
0,50MAX |
1.90-2.60 |
0.87-1.13 |
|
* Ni 0,40 max; V 0,18–0,25; Cb 0,06–0,10; N 0,03–0,07; Al 0,04 max |
|||||||
Mechanische Eigenschaften von ASTM A199:
|
Stahlsorte |
Zugfestigkeit (Mpa) |
Streckgrenze (Mpa) |
Verlängerung (%) |
Härte HRB MAX |
|
ASTM A199 T4 |
415MIN |
170MIN |
30/22 |
85HRB MAX |
|
ASTM A199 T5 |
415MIN |
170MIN |
30/22 |
85HRB MAX |
|
ASTM A199 T9 |
415MIN |
170MIN |
30/22 |
85HRB MAX |
|
ASTM A199 T11 |
415MIN |
170MIN |
30/22 |
85HRB MAX |
|
ASTM A199 T22 |
415MIN |
170MIN |
30/22 |
85HRB MAX |